Performance Characteristics:
Air-cooled hardening hot work die steel. good toughness, thermal fatigue resistance and abrasion resistance, and high hardenability.
Applications:
hot extrusion moulds and mandrels、forging mould of die-casting hammer; high-speed precision forging mould with inserts; die forging presses mould as well aluminum alloy die-casting mould, etc.
Chemical Composition(%):
C :0.32~0.45 Si:0.80~1.20
Mn:0.20~0.50 S :≤0.030
P :≤0.030 Cr:4.75~5.50
Ni: ≤0.25 Cu: ≤0.30
V :0.80~1.20 Mo:1.10~1.75
Process:
EAF+LF+VD+ESR+ Forged+ Annealed+Grinded/Machined
Annealed: 860-890°C, hardness ≤229HB
Quenching: 1020-1050°C, oil cooling or air cooling
Tempering: 560-580°C, hardness: 47-49HRC, twice tempering
Surface condition: black , grinded or machined/ turned.