Steel
|
|
C
|
Mn
|
Si
|
P
|
S
|
Cr
|
Mo
|
Ni
|
N
|
2205 (S31803
|
Min
|
-
|
-
|
-
|
-
|
-
|
21.0
|
2.5
|
4.5
|
0.08
|
Max
|
0.030
|
2.00
|
1.00
|
0.030
|
0.020
|
23.0
|
3.5
|
6.5
|
0.20
|
|
2205 (S32205
|
Min
|
-
|
-
|
-
|
-
|
-
|
22.0
|
3.0
|
4.5
|
0.14
|
Max
|
0.030
|
2.00
|
1.00
|
0.030
|
0.020
|
23.0
|
3.5
|
6.5
|
0.20
|
Density
|
7805 kg/m3
|
Elastic modulus
|
200 GPa
|
Mean coefficient of thermal expansion (μm/m/oC)
|
13.7 at 0-100oC
|
14.7 at 0-315oC
|
|
Thermal Conductivity (W/m.K)
|
19 at 100oC
|
Specific Heat 0-100oC( J/kg.K)
|
450
|
Electrical Resistivity (nΩ.m)
|
850
|
Steel
|
Tensile strength, Mpa
|
Yield strength, Mpa
|
Elongation %
|
Hardness
|
|
2205
|
620
|
450
|
25
|
31 C
|